Your Quotation Says 30% Recycled. The Real Number Is in the Nozzle.

Published guidance on how much scrap a magnesium charge may contain ranges from 10% to 80%. A foundry study measures what that ratio actually costs: 120,000 shots down to 45,000.
Ask a magnesium die caster how much of the charge is recycled material and you may be told 10 per cent, 30 per cent, 50 per cent or 80 per cent. All four numbers appear in current published material, and none of them is necessarily wrong, because they are not all answering the same question. What none of them answer is the question a buyer actually pays for: what does that ratio do to the part, and what does it do to the machine that makes the part.
Where the four numbers come from
YS/T 695-2025, the Chinese industry standard for wrought magnesium and magnesium alloy rectangular ingots, was published on 19 August 2025 and took effect on 1 March 2026, replacing the 2009 edition. Its quality-assurance appendix states that recycled material can generally be added at 10% to 30%, that it should meet the Class I block scrap requirements of GB/T 20926, and that for high-demand applications such as military or 3C plate and strip, recycled material should be avoided because it lowers finished yield. That standard addresses billet for forging and rolling, not die castings.
A purchasing guide for recycled magnesium ingots gives 30% to 50% as the sensible addition range and then makes a distinction that matters more than the range itself: experienced foundries put recycled material into non-load-bearing parts such as housings and brackets, and keep primary ingot, or a much lower addition, for anything that carries load. A melting reference gives the composition rule differently, as a ceiling rather than a target: Class I and Class II returns together must not exceed 80% of the charge mass, and Class II with Class III must not exceed 40%. The Magnetic Recycling Industry's own guidelines on die casting alloys conclude that at least 20% to 25% of clean die casting scrap can be added to primary ingot without deterioration in casting performance, and show scrap additions from 11% to 41% having very little effect on mechanical properties or corrosion behaviour across MRI 230D, AZ91D and AM60B, provided the MgO content stays below 600 ppm.
None of those sources contradicts another. They are talking about wrought billet, about general purchasing, about a charge ceiling, and about clean internal scrap respectively. The problem for a buyer is that all four are quoted without saying which one they mean, and the ratios are quoted without the grading that makes them meaningful.
The grading that has to travel with the ratio
GB/T 20926-2007 divides magnesium and magnesium alloy scrap into three classes and nine grades, each with a designation code. Class I is block material: new die casting scrap such as MDA21 and MDA22, used recovered die casting scrap as MDB41 through MDB57, casting scrap as MCA, and wrought forms as MWA and MWB. Class II is chips and turnings: dry machined turnings MTD61 and MTD62, non-dry turnings carrying oil or water as MTW71 through MTW74, and mixed-alloy turnings as MTM81 and MTM82. Class III is residue, MOS91 without salt and MOS92 with salt. A separate recycling specification for magnesium alloy die casting block scrap puts the recoverable yield of Class I at not less than 95%, Class II at above 80% and Class III below 80%.
So a ratio of 30% means nothing on its own. Thirty per cent of what grade, from which process, and what was it before it was scrap, decides the answer. The same document also requires that different grades not be mixed in transport, that bags or iron drums be used, that the marking carry the class, grade, alloy designation, weight and date, and that the buyer re-inspect within five days of receipt, with disputes raised in writing within fifteen.
What the ratio does to the metal
Two published studies point in the same direction and neither of them is a simple "recycled is worse" story.
In the first, an AZ91 study run as part of the RecMag project cast the same part with 0% and with 75% circulating scrap. The 75% group reached a mean ultimate tensile strength of 153 MPa against 128 MPa for the pure-ingot group, with yield strength rising from 79 to 106 MPa, and elongation falling from 1.5% to 1.3%. Hardness peaked at about 80 HB at 25% and 50% additions and dropped to roughly 70 HB at 75%, attributed to excessive Mg2Si, with Mg17Al12 identified as a brittle phase that is harmful if it forms a continuous network along grain boundaries. The authors attribute the strength gain to fine submicron impurity particles acting as nucleating agents, and note that it needs further confirmation.
In the second, a 2018 study in Archives of Foundry Engineering on AZ91 hardware wear gave the mechanical trends and the cost of them in the same table. Tensile strength rose as scrap content increased to 50% and then declined; elongation decreased steadily with every increase in scrap. The finding nobody quotes in a marketing paragraph was the hardware: the siphon, one of the most expensive consumables on a hot-chamber machine, fell from 120,000 injections at 100% virgin material to 45,000 at 100% scrap, a 62.5% reduction. The injection nozzle went from 55,000 to 20,000, the plunger from 80,000 to 35,000 and the sliding rings from 25,000 to 10,000. The mechanism was abrasive wear from hard non-metallic inclusions, specifically magnesium and aluminium oxides carried in with the scrap. The study's practical conclusion is that a scrap content around 50% is the ceiling for balancing material cost against manageable wear.
Read together, the two studies say something more precise than "recycled is bad". Moderate additions of clean, well-graded internal scrap can raise strength, partly through grain refinement. What falls, reliably and from the first increment, is elongation. And what falls alongside it, and which never appears on a material certificate, is the life of the pressure chamber hardware that has to carry the same oxides.
What the scrap actually costs at the receiving end
On the buying side, the checks that determine whether a batch is usable are specific. AZ91D has a specified aluminium range of roughly 8.3% to 9.7%, and a purchasing guide treats a batch-to-batch aluminium swing beyond plus or minus 0.5% as grounds for downgrading the material. Hydrogen content is checked separately, because recovered material generally carries more hydrogen than primary ingot and hydrogen in the melt shows up as gas porosity in the casting. Inclusions are assessed metallographically, which is why a low-grade batch ends up costing more in testing than it saves in metal.
The upstream side has its own burden. Recovered magnesium that goes through casting and machining brings back oil, water and foundry sand with it, and the treatment required before it can be recycled is a real cost line rather than a rounding error. Magnetic alloy residue with entrained oil has to be treated before landfill and carries its own handling constraints. These are the reasons a foundry with a clean internal scrap stream can sustain a higher ratio than a buyer purchasing recycled ingot from outside.
Three questions for a quotation
Stated as questions that can be answered:
What recycled proportion is used for this part number, at which grade under GB/T 20926, and is the recycled material internal loop material from your own runners and rejects or purchased ingot? What does your furnace record show for composition by heat number, including the recycled fraction in each heat, and what are the batch limits for aluminium, manganese, zinc and the copper and nickel that drive corrosion? And what does that recycled proportion do to your consumable replacement cycle, stated as injections or as months, since a siphon that runs from 120,000 shots to 45,000 is a line-cost item that belongs in the price.
We run tooling, die casting, precision machining and surface treatment in one plant in Ningbo, which means the runners and rejects our own lines produce come back to our own furnace, graded and weighed separately, and that we can give composition by heat number rather than a supplier's average. We would rather state the ratio for a specific part than quote a house percentage for the whole plant, because the honest answer differs between a housing and a bracket. Send the part and the alloy and we will tell you which of the three questions we can answer with records. Process scope here. For the other side of the same incoming-material question, see our note on export paperwork and alloy chemistry; for the inclusions that end up inside the casting, what an X-ray callout does and does not specify; and for why the gating system has to be designed around the same inclusions, our note on gating ratios.
The one-line version
A recycled percentage is a material cost decision that arrives as a mechanical property change and a tooling cost. The buyer who asks about the first and not the second gets the quotation with the interesting part removed.